Fatigue failure is the fracture of a part under repeated (cyclic) loading at stress levels well below its yield strength. A crack starts at a small stress raiser, grows a little with every cycle, and the part breaks suddenly when the remaining section can no longer carry the load. An S-N curve (also called a Wöhler curve) plots stress amplitude against the number of cycles to failure, and it is the basic tool for estimating fatigue life. For many steels the curve flattens near 106 to 107 cycles at the endurance limit; aluminium alloys generally show no true flattening.
This guide explains the ideas in plain English, then works through a shaft example with numbers checked in Python. It is educational material, not a substitute for testing or design standards.
Why parts fail below yield under repeated loading
A static tensile test tells you the load that yields or breaks a part in one pull. Real machine parts such as axles, crankshafts, gear teeth, springs and bolts see the same load again and again. Even when the nominal stress is far below yield, tiny regions at the surface, such as a scratch, a sharp corner or an inclusion, carry much higher local stress. In those spots the metal slips microscopically on each cycle. Over thousands or millions of cycles, that slip builds into a crack.
This is why fatigue is dangerous: the part shows little or no visible plastic deformation beforehand, and the final break can be sudden. It is commonly cited as a major cause of in-service failures of metal components, so every rotating or vibrating part deserves a fatigue check.
The three stages of fatigue failure
- Crack initiation. A microscopic crack forms at the surface or at a defect, usually where local stress is highest.
- Crack propagation. The crack grows a tiny amount per cycle. On the fracture surface this often leaves curved beach marks (also called clamshell marks), which look like ripples on a beach and point back toward the origin.
- Final fracture. When the uncracked area is too small to carry the load, the part fractures suddenly. This zone often looks rough or granular, compared with the smoother, beach-marked growth zone.
Inspecting a failed shaft for beach marks and locating the origin is one of the most useful practical skills in failure analysis.
Cyclic stress terms you must know
For a constant-amplitude cycle, the following quantities describe the loading. All are in MPa.
| Term | Symbol | Definition |
|---|---|---|
| Maximum stress | σmax | Highest stress in the cycle |
| Minimum stress | σmin | Lowest stress in the cycle |
| Stress range | Δσ | σmax − σmin |
| Stress amplitude | σa | (σmax − σmin) / 2 |
| Mean stress | σm | (σmax + σmin) / 2 |
| Stress ratio | R | σmin / σmax |
A rotating shaft under steady bending sees fully reversed stress: σm = 0 and R = −1. A load that goes from zero to a maximum and back has R = 0. As an example, a cycle from −100 MPa to +200 MPa has σa = 150 MPa, σm = 50 MPa and R = −0.5.
The S-N (Wöhler) curve
To build an S-N curve, many identical polished specimens are tested at different stress amplitudes until they break. Each result is one point: stress amplitude on the vertical axis, cycles to failure N on the horizontal axis, usually on logarithmic scales. Test results scatter widely, so a real curve is a statistical line (for example 50% survival) with scatter bands.
Low-cycle versus high-cycle fatigue
Roughly, low-cycle fatigue covers failures below about 103 to 104 cycles, where significant plastic strain occurs and strain-based methods (ASTM E606 testing) are used. High-cycle fatigue covers longer lives where stresses stay mostly elastic and stress-based S-N methods work well (ASTM E466 covers force-controlled testing). The boundary is approximate and varies by author and material.
Endurance limit
As general engineering knowledge, many ferrous metals (steels) show a knee in the S-N curve at roughly 106 to 107 cycles. Below the stress at that knee, called the endurance limit Se, the specimen is expected to last effectively indefinitely under constant-amplitude loading. Aluminium alloys and many other non-ferrous metals do not show a true limit. Their curves keep sloping down, so designers quote strength at a chosen life, often 5 × 108 cycles. Corrosion, overloads and variable amplitudes can also remove the apparent limit in steels.
A common rule of thumb from Shigley’s textbook, for steels with ultimate strength Sut up to about 1,400 MPa, is Se′ ≈ 0.5 Sut for a small polished test specimen. Treat this as an estimate only. Use measured data where available.
Adjusting the endurance limit: Marin factors
A lab specimen is small, polished and loaded in a clean way. Your component is not. Marin modification factors scale the specimen value to the real part:
Se = ka · kb · kc · kd · ke · Se'
- ka (surface): ground, machined, hot-rolled and forged surfaces are progressively worse than polished.
- kb (size): larger sections generally have lower endurance limits.
- kc (load): bending, axial and torsion loading give different effective limits.
- kd (temperature): strength changes at elevated temperature.
- ke (reliability): higher required reliability lowers the usable value, because test data scatter.
Shigley gives empirical equations for these factors. For a machined surface it uses ka = 4.51 Sut−0.265 (Sut in MPa), and for bending or torsion of a round shaft of diameter d in mm (2.79 to 51 mm), kb = 1.24 d−0.107. Check the current edition for the exact ranges before you rely on them.
Stress concentration and notch sensitivity
Shoulders, keyways, holes and grooves raise local stress. The theoretical factor Kt comes from geometry charts or FEA. Real materials are usually less sensitive than theory predicts, so a notch sensitivity q (between 0 and 1) gives the fatigue stress concentration factor:
Kf = 1 + q (Kt − 1)
You then multiply the nominal alternating stress by Kf. Sharp notches in strong materials have q closer to 1, so they hurt most.
Mean stress and the Goodman line
A tensile mean stress reduces the allowable amplitude. The modified Goodman line joins Se on the amplitude axis to Sut on the mean-stress axis. For infinite life the safe condition, expressed as a factor of safety n, is:
σa / Se + σm / Sut = 1 / n
Goodman is conservative and commonly used in teaching. Other criteria (Gerber, Soderberg, Morrow, Smith-Watson-Topper) exist, and the best choice depends on the material and on available test data.
Finite life: the Basquin relation
Between roughly 103 and the endurance knee, the S-N line is approximately straight on log-log axes. The Basquin relation describes it:
σa = σf′ (2N)^b
Here σf′ is the fatigue strength coefficient, b is the fatigue strength exponent (typically negative, often between about −0.05 and −0.15 for metals), and 2N is reversals to failure. A practical version used in Shigley’s is Sf = a Nb, where a = (f Sut)² / Se and b = −(1/3) log10(f Sut / Se). Here f is the fraction of Sut at 103 cycles, often taken near 0.9 for steels of this strength.
Miner’s rule for variable loading
Real parts rarely see one constant amplitude. The Palmgren-Miner linear damage rule sums the fraction of life used at each level:
D = Σ (ni / Ni) and failure is predicted when D ≈ 1
For example, 2 × 105 cycles at a level whose life is 106, plus 105 cycles at a level whose life is 5 × 105, gives D = 0.2 + 0.2 = 0.4, so about 60% of life remains. Miner’s rule ignores load sequence effects and has real scatter, so many designers use a limit of D below 1.
Worked example: a steel shaft in fully reversed bending
Assumptions (illustrative, not a real design): round shaft, diameter d = 30 mm, steel with Sut = 600 MPa, machined surface, 99% reliability, room temperature, fully reversed bending moment, shoulder fillet with Kt = 1.7 and notch sensitivity q = 0.85.
Step 1: Estimate Se. Se′ = 0.5 × 600 = 300 MPa. Then ka = 4.51 × 600−0.265 = 0.828; kb = 1.24 × 30−0.107 = 0.862; kc = kd = 1; ke = 0.814 (99% reliability in Shigley’s table). So Se = 0.828 × 0.862 × 1 × 1 × 0.814 × 300 ≈ 174 MPa.
Step 2: Infinite-life check. Kf = 1 + 0.85 × (1.7 − 1) = 1.595. For M = 180 N·m, nominal bending stress σ = 32M / (π d³) = 67.9 MPa, so σa = 1.595 × 67.9 = 108.3 MPa. With σm = 0, n = Se / σa = 174.2 / 108.3 ≈ 1.61.
Step 3: Add a mean stress. If an additional steady tensile mean stress of 100 MPa were present (hypothetical), Goodman gives 1/n = 108.3/174.2 + 100/600 = 0.789, so n ≈ 1.27. Notice how mean stress lowers the safety margin.
Step 4: Finite life. Suppose the moment is raised to M = 400 N·m (hypothetical overload). Then σa = 1.595 × 32 × 400 / (π × 0.030³) ≈ 240.7 MPa, which is above Se, so life is finite. Using f = 0.9: a = (0.9 × 600)² / 174.2 ≈ 1,674 MPa, b = −(1/3) log10(540 / 174.2) ≈ −0.164. Solving N = (σa / a)1/b gives about 1.4 × 105 cycles. The constants here come from the textbook construction with assumed f and Se, so this is a rough estimate with large scatter, not a prediction.
Python snippet: compute life and draw the S-N curve
import math
import numpy as np
import matplotlib.pyplot as plt
# Illustrative inputs (MPa)
Sut, Se, f = 600.0, 174.2, 0.9
M, d, Kf = 400.0, 0.030, 1.595 # N*m, m, dimensionless
a = (f * Sut) ** 2 / Se
b = -math.log10(f * Sut / Se) / 3
sigma_a = Kf * 32 * M / (math.pi * d ** 3) / 1e6 # MPa
N = (sigma_a / a) ** (1 / b)
print(f"sigma_a = {sigma_a:.1f} MPa, N = {N:.3g} cycles")
n = np.logspace(3, 7, 200)
S = np.where(n < 1e6, a * n ** b, Se) # knee at 1e6 for steel
plt.loglog(n, S, label="Estimated S-N line (illustrative)")
plt.axhline(sigma_a, ls="--", color="grey", label="Applied amplitude")
plt.xlabel("Cycles to failure N")
plt.ylabel("Stress amplitude (MPa)")
plt.grid(True, which="both", alpha=0.3)
plt.legend()
plt.savefig("sn_curve.png", dpi=150)
Running this reproduces the numbers above: σa ≈ 240.7 MPa and N ≈ 1.39 × 105 cycles.
Practical design tips
- Use generous fillet radii at shoulders. Sharp internal corners are the most common fatigue origin.
- Specify a good surface finish and avoid tool marks, nicks and corrosion pits.
- Consider surface treatments such as shot peening or case hardening, which can introduce helpful compressive residual stress. Benefit depends on process control.
- Avoid keyways, cross-holes and abrupt diameter changes near high-bending regions, or use sled-runner or profiled keyways where needed.
- Avoid unexpected tensile mean stress from assembly preload or residual stress, and keep welds away from high-stress areas.
- Protect against corrosion, which can reduce fatigue strength substantially.
Limitations
Everything above is a simplified model. Real fatigue life depends on material batch, manufacturing, environment, residual stress, loading sequence and inspection. Scatter of a factor of ten or more in life is normal. Safety-critical parts such as aircraft, pressure equipment, lifting gear and vehicle components require testing, applicable codes and standards, and review by a qualified engineer. This article is educational only and is not professional engineering advice.
FAQ
Is the endurance limit the same as yield strength?
No. The endurance limit for steels is usually well below yield, often near half of the ultimate strength for a polished specimen, and it applies to cyclic loading.
Do all metals have an endurance limit?
No. Steels commonly show one under benign conditions. Aluminium and many other non-ferrous alloys generally do not, so designers specify fatigue strength at a chosen number of cycles.
Why is my real part weaker than the S-N data?
Published curves usually come from small polished specimens. Surface finish, size, notches, corrosion and reliability targets all reduce the usable value.
How many cycles count as infinite life?
For steels the convention is often about 106 to 107 cycles. Non-ferrous metals use a stated design life such as 108 cycles or more.
Sources to check
- Shigley’s Mechanical Engineering Design (Budynas and Nisbett), fatigue chapter
- Dowling, Mechanical Behavior of Materials
- Suresh, Fatigue of Materials
- ASTM E466, standard practice for force-controlled constant amplitude axial fatigue tests of metallic materials
- ASTM E606, standard test method for strain-controlled fatigue testing
Numbers and factors quoted here are textbook rules of thumb and should be confirmed against the current edition of your reference.
Every formula you need, in one place
The Mechanical Engineering Formula Handbook covers 140+ core formulas across 12 subjects, with symbols, SI units and notes on when to use each one. Ideal for exams and quick checks at work. Want the full kit? The Engineer Toolkit Bundle adds calculators, Excel practice and AI prompts for engineers.
Prefer video? Watch the tutorials on YouTube · Browse all toolkits